鑫洋公司锶钡铁氧体预烧料磁性能
|
牌号
|
Br
|
|
Hcb
|
|
Hcj
|
|
(BH)max
|
|
TYPE
|
Mt
|
Gs
|
KA/m
|
Koe
|
KA/m
|
Koe
|
KJ/m3
|
mGOe
|
BNY25
|
360-380
|
3.6-3.8
|
150-180
|
1.85-2.26
|
160-290
|
2.0-2.38
|
22.5-25
|
2.8-3.1
|
SMY28
|
380-440
|
3.8-4.4
|
180-200
|
2.26-2.5
|
190-220
|
2.38-2.76
|
25.0-30.0
|
3.1-3.8
|
SM30H-1
|
370-390
|
3.7-3.9
|
205-240
|
2.57-3.0
|
220-255
|
2.76-3.2
|
25.0-28.5
|
3.1-3.6
|
SM20H-2
|
400-440
|
4.0-4.4
|
220-240
|
2.3-2.5
|
230-250
|
2.9-3.15
|
31.0-34.0
|
3.8-4.2
|
SM30H-2
|
400-420
|
4.0-4.2
|
280-295
|
3.52-3.7
|
318-335
|
4.0-4.2
|
31.0-35.0
|
3.9-4.4
|
SM33
|
410-430
|
4.1-4.3
|
220-250
|
2.77-3.14
|
225-255
|
2.83-3.21
|
31.5-35
|
4.0-4.4
|
SM35
|
400-410
|
4.0-4.1
|
175-195
|
2.2-2.45
|
180-200
|
2.26-2.51
|
30.0-32.0
|
3.8-4.4
|
鑫洋牌烧结永磁铁氧体磁体的磁特性
|
牌号
|
SJ-T1014
|
Br
|
|
Hcb
|
|
Hcj
|
|
(BH)max
|
|
参照标准
|
TYPE
|
|
mT
|
KGS
|
KA/M
|
Koe
|
KA/M
|
Koe
|
KJ/m3
|
MGOe
|
Eqvivalent foreigh Standart
|
XY-1
|
Y28-1
|
380-410
|
3.8-4.1
|
130-175
|
1.63-2.20
|
135-158
|
1.7-2.33
|
25.0-30.0
|
3.1-3.8
|
IEC-25/14
|
XY-2
|
Y28-2
|
370-400
|
3.7-4.0
|
175-210
|
2.20-2.64
|
180-220
|
2.26-2.77
|
26.0-30.0
|
3.3-3.8
|
IEC-26/18
|
XY-3
|
Y30H-1
|
390-410
|
3.9-4.1
|
240-270
|
3.02-3.39
|
240-285
|
3.02-3.58
|
28.0-32.5
|
3.5-4.1
|
TDK-FB4B
|
XY-4
|
Y30H-2
|
395-415
|
3.95-4.15
|
275-300
|
3.46-3.77
|
310-335
|
3.90-4.21
|
28.5-32.0
|
3.5-4.0
|
TDK-5H
|
XY-5
|
Y32
|
400-420
|
4.0-4.2
|
160-190
|
2.01-2.88
|
160-195
|
2.01-2.45
|
30.0-33.5
|
3.8-4.2
|
TDK-FB4A
|
XY-6
|
Y33
|
410-440
|
4.1-4.3
|
220-250
|
2.77-3.14
|
225-255
|
2.83-3.21
|
31.5-35.0
|
4.0-4.4
|
TDK-FB4X
|
永磁铁氧体的物理特性(室温)
|
铁氧体类别
|
Sr0.6Feo
|
Bs0.6Feo
|
饱和磁化强度Ms
|
370Gs
|
380Gs
|
各项异性场Ha
|
20KOe
|
17KOe
|
居里温度θf
|
460℃
|
450℃
|
理论密度d
|
5.11g/cm
|
5.28g/cm
|
比热
|
0.2cal/g.℃
|
0.2cal/g.℃
|
电阻率ρ
|
≥10.cm
|
≥10.cm
|
可逆温度系数ΔBr/Br
|
+0.38-0.5%℃
|
0.38-0.5%℃
|
相对可逆磁导率Mree
|
1.05-1.2
|
1.05-1.2
|
可逆温度系数ΔJHc/JHc
|
-0.18%/℃
|
0.18%/℃
|
热膨胀系数//c轴
|
15×10-6K
|
15×10-6K
|
⊥c轴
|
10×10-6K
|
10×10-6K
|
|